摩擦摩損特性一覽表
性能項目
測試條件
測試方法
數(shù)值/描述
單位
機(jī)械性能
拉伸強(qiáng)度(引張強(qiáng)度)
ASTM D638/ISO 527
54
kg/cm²(MPa)[Lb/in2]
斷裂伸長率
ASTM D638/ISO 527
35*
%
拉伸模量
ASTM D638/ISO 527
kg/cm²(MPa)[Lb/in2]
拉伸屈服伸長率(延伸率)
ASTM D638/ISO 527
%
拉伸斷裂伸長率(延伸率)
ASTM D638/ISO 527
%
彎曲模量(彎曲彈性率)
ASTM D790/ISO 178
2200
kg/cm²(MPa)[Lb/in2]
彎曲強(qiáng)度
ASTM D790/ISO 178
75
kg/cm²(MPa)[Lb/in2]
洛氏硬度
ASTM D785
IZOD 缺口沖擊強(qiáng)度
1/4" 23℃
ASTM D256/ISO 179
kg·cm/cm(J/M)ft·lb/in
1/4" -30℃
ASTM D256/ISO 179
kg·cm/cm(J/M)ft·lb/in
1/8" 23℃
ASTM D256/ISO 179
kg·cm/cm(J/M)ft·lb/in
1/8" -30℃
ASTM D256/ISO 179
kg·cm/cm(J/M)ft·lb/in
Charpy沖擊強(qiáng)度
23℃ (缺口)
ASTM D256/ISO 179
kg·cm/cm(J/M)ft·lb/in
-30℃(缺口)
ASTM D256/ISO 179
kg·cm/cm(J/M)ft·lb/in
23℃(無缺口)
ASTM D256/ISO 179
kg·cm/cm(J/M)ft·lb/in
-30℃(無缺口)
ASTM D256/ISO 179
kg·cm/cm(J/M)ft·lb/in
物性性能
比重(密度)
ASTM D792/ISO 1183
1.37
成型收縮率
ASTM D955
%
熔融指數(shù)(流動系數(shù))
200℃/5kg
ASTM D1238/ISO 1133
g/10min
220℃/10kg
ASTM D1238/ISO 1133
g/10min
吸水率 23℃/24H
ASTM D570/ISO 62
%
熱性能
熱變形溫度
退火
ASTM D648/ISO 75
℃(℉)
未退火
ASTM D648/ISO 75
℃(℉)
維卡軟化點
ASTM D1525/ISO R306
℃(℉)
熔點
-
℃(℉)
燃燒性(率)
UL94
線性膨脹系數(shù)
ASTM D696/ISO 11359
13
mm/mm.℃
電氣性能
介電常數(shù)
100HZ
ASTM D150/IEC 60250
1MHZ
ASTM D150/IEC 60250
體積電阻率
ASTM D257/IEC 60093
3.0*10
Ω.cm
表面電阻率
ASTM D257/IEC 60093
3.0*10
Ω
耐電弧性
ASTM D495/IEC 60112
加工條件
干燥條件
加工溫度
射嘴
℃
料筒前段
℃
料筒中段
℃
料筒后段
℃
熔體溫度
℃
模具溫度
℃
壓力
注塑壓力
Mpa
保壓壓力
Mpa
背壓
Mpa
螺桿轉(zhuǎn)速
rpm
其他
備注
顏色
特性
用途
對碳素鋼 | 對標(biāo)準(zhǔn)POM (M90-44) | 對同樣的塑料 | ||||||||||
評價 條件 |
摩損量比 (×10-3 mm3/N·km) |
動摩擦系數(shù) | 評價 條件 |
摩損量比 (×10-3 mm3/N·km) |
動摩擦系數(shù) | 評價 條件 |
摩損量比 (×10-3 mm3/N·km) |
動摩擦系數(shù) | ||||
評價塑料方面 | 炭素鋼方面 | (μD) | 評價塑料方面 | M90-44方面 | 總量 | (μD) | 總量 | (μD) | ||||
M90-44 | A | 0.30 | < 0.01 | 0.40 | - | D | 100 | 0.37 | ||||
B | 0.65 | < 0.01 | 0.46 | |||||||||
C | 0.90 | < 0.01 | 0.52 | |||||||||
AW-01 | A | 0.20 | < 0.01 | 0.16 | D | 7.0 | 14.0 | - | 0.30 | D | 8.0 | 0.22 |
JW-03 | A | 0.21 | < 0.01 | 0.17 | D | 0.8 | 2.2 | - | 0.21 | D | 4.0 | 0.22 |
NW-02 | A | 0.19 | < 0.01 | 0.17 | D | 3.0 | 10.0 | - | 0.37 | D | 4.0 | 0.29 |
SW-01 | A |
0.16 |
< 0.01 | 0.14 | D | 4.0 | 9.0 | - | 0.21 | D | 3.0 | 0.18 |
SW-41 | A | 0.70 | < 0.01 | 0.20 | D | 0.8 | 1.3 | - | 0.17 | D | 3.0 | 0.10 |
SW-22 | A | 0.22 | < 0.01 | 0.20 | D | 3.0 | 4.5 | - | 0.19 | D | 7.0 | 0.13 |
YF-10 | A | 0.60 | < 0.01 | 0.20 | D | 8.0 | 65.0 | - | 0.32 | D | 4.0 | 0.24 |
YF-20 | A | 0.60 | < 0.01 | 0.18 | D | 5.0 | 35.0 | - | 0.32 | D | 4.0 | 0.22 |
TR-20 | B | 80.0 | 1.50 | 0.56 | D | 5.0 | 70.0 | - | 0.34 | D | 90 | 0.37 |
KT-20 | B | 25.0 | < 0.01 | 0.36 | D | 2.0 | 40.0 | - | 0.35 | D | 50 | 0.38 |
GH-25 | B | 80.0 | 4.00 | 0.60 | D | 3.0 | 100.0 | - | 0.37 | D | 80 | 0.33 |
GB-25R | B | 70.0 | 5.00 | 0.51 | D | 0.4 | 80.0 | - | 0.37 | D | 25 | 0.35 |
CH-20 | B | 3.00 | 0.05 | 0.24 | D | 0.5 | 100.0 | - | 0.35 | D | 3.5 | 0.21 |
EB-10 | A | 0.60 | < 0.01 | 0.52 | D | 2.0 | 57.0 | - | 0.36 | D | 18 | 0.38 |
ES-5 | A | 0.80 | < 0.01 | 0.47 | D | 12.0 | 40.0 | - | 0.43 | D | 40 | 0.50 |
EW-02 | A | 1.00 | < 0.01 | 0.34 | D | 2.0 | 80.0 | - | 0.34 | D | 60 | 0.34 |
評價條件 | A | 面壓: 0.98MPa / 線速度: 30cm/s | |
B | 面壓: 0.49MPa / 線速度: 30cm/s | ||
C | 面壓: 0.25MPa / 線速度: 30cm/s | ||
D | 面壓: 0.06MPa / 線速度: 15cm/s |